UV Varnish Performance Testing Items and Methods
Release time:
2014-07-03 14:51

UV Varnish Performance Testing Items and Methods
I. Basic Appearance Requirements
1. The gloss coating has excellent leveling properties and exhibits no orange-peel or ripple effects.
2. The paint has excellent coverage (oil resistance). After spraying, there should be no oil stains, oil spots, depressions, white spots, or any other similar defects; furthermore, there should be no fogging phenomenon.
3. Good glossiness, with a requirement of >90.
II. Performance Testing Requirements
| Serial number | Test item | Testing Methods and Requirements |
| 1 | Adhesion Test | Use a knife to score the surface of the paint film with a grid of 10×10 squares, each measuring 1 mm × 1 mm. The depth of the cuts should be sufficient to expose the substrate. Use a brush to carefully remove any debris from the test area. Apply the test tape perpendicularly and firmly onto the paint film surface, ensuring that the tape is smooth and free of air bubbles. After letting it sit for 1 minute, quickly peel off the tape. Repeat this test five times at the same location, checking whether the UV oil has peeled off. The test must meet the 5B requirement. |
| 2 | Hardness test | Using a pencil (Mitsubishi brand), first sharpen the lead into a cylindrical shape and then smooth it out on 400-grit sandpaper. Next, place the pencil onto a dedicated pencil hardness tester (with a load of 1 kg applied to the tip and the pencil held at a 45-degree angle to the horizontal plane). Push the pencil forward approximately 56 mm, making a total of five strokes. Then, erase the marks cleanly with an eraser and inspect the product surface for any traces. If no obvious scratches are found, the product is considered qualified. |
| 3 | Bending test | Bend the product forward by 90 degrees three times, and no paint chipping or peeling is allowed. |
| 4 | RCA Abrasion Test | Using a dedicated paper tape testing machine with a 175g load, the total test cycle shall consist of either 300 or 500 cycles. The test is considered合格 (pass) if no bottom-through leakage occurs. |
| 5 | High-voltage withstand test | Require passing a high voltage of 8,000V to ensure no electrical leakage (applicable only to plastic substrates). |
| 6 | Salt Spray Resistance Test | The salt solution is prepared using sodium chloride (chemically pure or analytically pure) and distilled water, with a concentration of 5 ± 0.1%. The pH value of the salt solution before atomization should be between 6.5 and 7.2. The test temperature is 35 ± 2 degrees Celsius. The continuous atomization duration is 48 hours. During inspection, no signs of bubbling, cracking, discoloration, UV degradation, or coating peeling shall be observed. |
| 7 | Impact strength | Under a force of 50 kg both forward and backward, after impact, the paint film shows no diffusion or water-ring-like cracks, no radial cracks (except those caused by cracking of the substrate due to spraying), and no flaking. The impact was repeated three times. |
| 8 | Alcohol-resistant test | Thoroughly dip a piece of pure cotton cloth into anhydrous alcohol (concentration >99.5%), wrap it around a dedicated 1000g weight, and rub it back and forth across the sample surface at a speed of 40 to 60 strokes per minute for 300 cycles. The test is considered合格 (pass) if the underlying substrate remains completely concealed. |
| 9 | Oil resistance | Drop 2–5 drops of No. 150 machine oil onto the paint film, let it sit for 24 hours, and if there are no obvious abnormalities in the paint film, it is considered qualified. |
| 10 | Water resistance | Place half of the sample into tap water at 60°C and let it sit for 4 hours. Then, remove the sample, wipe off the surface water with a cloth, and immediately inspect the appearance of the paint film. The paint film should show no signs of bubbling, delamination, cracking, hazing, or discoloration, and its adhesion should reach 5B. |
| 11 | Water-resistant and boilable | Place the sample into boiling water at 100°C for 1 hour or into water at 80°C for 2 hours. The test requires no bubbling or cracking, and the adhesion test must achieve a rating of 5B. |
| 12 | Cosmetic-Resistant Testing | After applying sunscreen to the coating film surface, place the product in a constant-temperature chamber (temperature: 60°C ± 2°C, humidity: 90% ± 2% RH) and keep it there for 24 hours. Then, remove the product, wipe off any cosmetic residue with a cotton cloth, and inspect the outer surface for abnormalities. The adhesion and abrasion resistance tests should both pass successfully. |
| 13 | High-temperature resistance test | Under conditions of a temperature of 85°C ± 3°C, the sample shall be kept for 72 hours continuously, then left at room temperature for 2 hours before commencing the inspection. The appearance shall show no obvious defects, and adhesion must reach Grade 5B to be considered qualified. |
| 14 | Low-temperature resistance test | Under conditions of a temperature of -40°C ± 3°C, the sample shall be kept for 48 hours continuously, then left at room temperature for 2 hours before commencing the inspection. The appearance shall show no obvious defects, and adhesion must reach Grade 5B to be considered qualified. |
| 15 | Constant temperature and humidity testing | Under conditions of a temperature of 85°C ± 3°C and a humidity of 90% to 95%, the sample shall be kept for 48 hours continuously, then left at room temperature for 2 hours before testing begins. The inspection shall reveal no obvious defects in appearance, and adhesion must reach Grade 5B to be considered qualified. |
| 16 | Thermal Shock Test | Place the sample at a temperature of -40°C ± 3°C for 30 minutes, then place it at a high temperature of 85°C ± 3°C for another 30 minutes, with a transition time of 15 seconds. Perform 32 cycles of this procedure. After the test, allow the sample to stand at room temperature for 2 hours. The sample shall be considered qualified if no bubbling, peeling, or damage is observed on its surface. |
| 17 | Hand-sweat resistance test (Acidic) |
Place the dust-free cloth soaked in sweat onto the sample surface and seal it tightly with a plastic bag. In 1,000 ml of water, add 20 g of sodium chloride, 17.5 g of ammonium chloride, 5 g of urea, 2.5 g of acetic acid, and 15 g of lactic acid. Then, gradually add sodium hydroxide until the pH of the solution reaches 4.7. After keeping the sample under conditions of 65°C ± 2°C and 90% relative humidity for 48 hours, wipe clean the sweat from the sample surface, inspect the appearance of the paint film, and test the adhesion of the paint. The adhesion must meet the requirement of 5B. |
| 18 | Hand-sweat resistance test (Alkaline) |
Place the dust-free cloth soaked in sweat onto the sample surface and seal it tightly with a plastic bag. Then, add 4.2 g of sodium bicarbonate, 0.5 g of sodium chloride, 0.2 g of potassium carbonate, and 1000 ml of water, adjusting the pH to 8.8. After keeping the sample under conditions of 65°C ± 2°C and 90% relative humidity for 48 hours, wipe off the sweat from the sample surface, inspect the appearance of the paint film, and test the adhesion of the paint. The adhesion must meet the requirement of 5B. |
| 19 | The eraser is wear-resistant. | Using a dedicated eraser, apply a force of 500 g to the product surface, and perform reciprocating friction motions at a rate of approximately 40 to 60 cycles per minute for a total of 200 cycles. After the test is completed, the paint shall be considered合格 (pass) if there is no visible substrate showing through. |
| 20 | Age resistance | Natural Exposure Method: Take the cured UV varnish samples, cover half of them with white cardboard, and then expose them to sunlight. In summer, expose them for 7 days; in winter, expose them for 30 days. Artificial Aging Method: Place the cured UV varnish samples into an ultraviolet aging chamber and age them for 5 × 24 hours. The coating film is considered qualified if it shows no discoloration, bubbling, or cracking. |
Share to:
Related News
Evaluation and Quality Control of UV Resins
UV resin is an important polymer material widely used in fields such as printing, coatings, and adhesives. Quality control of UV resin is crucial to its application performance. This article will briefly introduce the evaluation methods and quality control measures for UV resin.
How to Enhance the Adhesion of UV Coatings
The adhesion of UV coatings is a critical factor affecting their spray-coating quality. In practical applications, differences in substrate materials, variations in coating thickness, and factors such as the power of UV curing can all lead to insufficient bonding between the coating and the substrate, resulting in issues like paint chipping and failure to pass testing. To address these problems, it is possible to enhance the adhesion between the coating and the substrate through appropriate pre-treatment measures.
What should I do if UV resin/coating exhibits gelation? And what are the precautions to take?
In the coatings industry, it’s common for some customers to report gelation issues with UV resins or UV coatings. There are multiple factors that can cause UV resin gelation, and when troubleshooting this problem, it’s important to systematically rule out each potential cause one by one. So, what should you do if your UV resin or UV coating experiences gelation? What precautions should you take? Let’s take a closer look at the causes of gelation below.