Overview of Acrylic Resin Design, Development, and Production Technologies


I. Overview of Acrylic Resins

1. Concept of acrylic resin

Acrylic resins are copolymers formed by the addition polymerization of monomers containing unsaturated double bonds, such as acrylates or methacrylates.

2. Structural Features

The resin main chain synthesized by copolymerization of unsaturated double-bond monomers consists of carbon-carbon single bonds, while the side chains feature ester structures.

The main chain exhibits a primary absorption peak for light that falls outside the solar spectrum range; therefore, the resulting acrylic coatings demonstrate excellent lightfastness and outstanding outdoor aging resistance. The presence of ester groups on the side chains prevents crystallization in acrylic coatings, while the versatility of these ester groups also enhances solubility in various media and compatibility with a wide range of resin types used in coatings.

3. Classification of Acrylic Resins

Based on coating formulation types, the main categories include: solvent-based coatings, waterborne coatings, high-solids coatings, and powder coatings.

Acrylic resins used in coatings are classified according to their film-forming properties into thermoplastic acrylic resins and thermosetting acrylic resins.

According to the method of production, polymerization can be classified into: solution polymerization, emulsion polymerization, suspension polymerization, and bulk polymerization.

4. Mechanism of Acrylic Polymerization Reaction

II. Acrylic Resin Design and Development

1. Basic Principles:

(1) The resin formulation—solvent-based or water-based—must be determined based on the specific substrate and product.

(2) Determine the monomer composition, glass transition temperature (Tg), solvent composition, type and amount of initiator, and polymerization process based on performance requirements.

(3) The optimal product process and formulation are determined through experimentation, followed by verification and refinement. Among these steps, the selection of monomers is the core component of formulation design.

2. Selection of monomers

(1) First, you need to become familiar with the monomer.

For ease of application, polymerizable monomers are typically categorized into three major types: hard monomers, soft monomers, and functional monomers.

a. Common hard monomers: methyl methacrylate (MMA), styrene (ST), acrylonitrile (AN);

Characteristics: Typically contains methyl groups, benzene rings, and carboxyl groups; has a very high glass transition temperature (around 100℃).

Function: To increase the hardness of the resin.

b. Common soft monomers: ethyl acrylate (EA), butyl acrylate (BA), 2-ethylhexyl acrylate (2-EHA), lauryl acrylate (LA), and others;

Characteristics: Typically features longer chain segments and a very low glass transition temperature (below -10℃);

Function: Enhance flexibility and promote film formation.

c. Common functional monomers: 2-hydroxyethyl acrylate (HEA), glycidyl methacrylate (GMA), acrylamide, vinyltrimethoxysilane, methacrylic acid, and others;

Features: Generally contains hydroxyl groups, carboxyl groups, amino groups, epoxy groups, silicon-containing groups, and fluorine-containing groups.

Function: Introduces functional groups or crosslinking sites to enhance adhesion, water resistance, solvent resistance, and other properties.

Specific characteristics of functional monomers:

a. Hydroxyl-containing monomers—such as HEA, HEMA, HPA, HPMA, and certain modified monomers—can provide functional groups for polyurethane curing agents and amino resin crosslinking in solvent-based resins.

b. Monomers containing carboxyl groups: acrylic acid, methacrylic acid, itaconic acid, etc. The introduction of carboxyl groups can enhance the resin’s wetting properties toward pigments and fillers as well as its adhesion to substrates. Moreover, these carboxyl groups are reactive with epoxy groups and exhibit catalytic activity in the curing of amino resins.

c. Silicone monomers: vinyl trimethoxysilane (YDH-171), γ-methacryloxypropyl trimethoxysilane (KH-570), etc. Vinylsiloxane monomers are highly reactive and readily undergo hydrolysis and crosslinking; therefore, their dosage should be kept low, and it is best to add them during the holding stage of the polymerization process.

(2) Special functional monomers

γ-Aminopropyltriethoxysilane (KH-550): NH2CH2CH2CH2Si(OCH2CH3)3

The structure of γ-glycidoxypropyltrimethoxysilane (KH-560) is as follows:

This type of silane coupling agent generally contains two functional groups: the epoxy group can react with hydroxyl, carboxyl, or amino groups on the resin, while the alkoxysilane moiety undergoes polycondensation via hydrolysis to form crosslinks. It is typically used as an externally added crosslinking agent in cold mixing applications.

Another class of relatively important monomers is tert-butyl vinyl carbonate. Tert-butyl carboxylic acid is a highly branched saturated acid with three alkyl substituents attached to the α-carbon, and its structural formula is as follows:

The epoxy group of glycidyl trimethylolpropane exhibits high reactivity. The most useful reactions for coating resins involve its interaction with hydroxyl, carboxyl, and amine groups. This high reactivity of the epoxy group enables it to incorporate into the macromolecular chains of polyester, alkyd, and acrylic resins even at conventional temperatures. The reaction is nearly quantitative, with minimal side reactions, thus providing a raw material basis for preparing high-solids-content coating resins that feature narrow molecular weight distributions and low viscosities.

Based on the influence of monomers on coating performance, monomers can often be categorized as follows for ease of application.

Monomer name Function
Methyl methacrylate
Ethyl methacrylate
Styrene
Acrylonitrile
Increase hardness—this is referred to as a hard monomer.
Ethyl acrylate
n-Butyl acrylate
Lauryl acrylate
2-Ethylhexyl acrylate
Lauryl methacrylate
n-Octyl methacrylate
Soft monomers are those that enhance flexibility and promote film formation.
Acrylic acid-2-hydroxyethyl ester
2-Hydroxypropyl acrylate
2-Hydroxyethyl methacrylate
2-Hydroxypropyl methacrylate
Glycidyl methacrylate
Acrylamide
N-Hydroxymethylacrylamide
N-Butoxymethyl (methyl)acrylamide
Diacetone Acrylamide (DAAM)
Ethyl acetoacrylate (AAEM)
Divinylbenzene
Vinyl trimethoxysilane
Vinyl triethoxysilane
Vinyl triisopropoxysilane
γ-Methacryloxypropyltrimethoxysilane
Introducing functional groups or crosslinking sites to enhance adhesion is referred to as a crosslinking monomer.
Lower alkyl esters of acrylic acid and methacrylic acid
Styrene
Anti-pollution performance
Methyl methacrylate
Styrene
Lauryl methacrylate
2-Ethylhexyl acrylate
Water resistance
Acrylonitrile
Butyl methacrylate
Lauryl methacrylate
Solvent resistance
Ethyl acrylate
n-Butyl acrylate
2-Ethylhexyl acrylate
Methyl methacrylate
Butyl methacrylate
Light retention and color retention
Acrylic
Methyl acrylate
Methylenesuccinic acid (itaconic acid)
Styrenesulfonic acid
Sodium vinyl sulfonate
AMPS
To achieve water solubility and enhance adhesion, these are referred to as water-soluble monomers and surface-active monomers.

3. Selection and proportioning of soft and hard monomers

Basic formulation = soft monomer + hard monomer + functional monomer

(1) Tg design (determining Tg)

Glass transition temperature: This is the lowest temperature at which the segments of a homopolymer chain can move. The greater the flexibility of the molecular chain, the lower the glass transition temperature; conversely, the greater the rigidity of the molecular chain, the higher the glass transition temperature.

Generally, the glass transition temperature of acrylic resin is determined based on comprehensive requirements such as the type, performance, and special properties of the coating. The specific circumstances are as follows:

a. The higher the Tg value, the harder the coating film (but note that the coating film must not be brittle); the stronger its scratch resistance.

b. The higher the Tg, the better the surface drying of the coating film after paint application and the better the solvent release performance.

c. The higher the Tg, the higher the final viscosity of the resin reaction;

d. The higher the Tg value, the better the solvent and corrosion resistance of the coating film after paint application.

e. Typically, the resin used in thermoplastic plastic paints for topcoats has a softening point generally above 70℃;

f. For plastic coatings used as primers, the glass transition temperature (Tg) of the resin should ideally be controlled within the range of 45–60℃.

g. For topcoats used on televisions, mobile phones, computers, and other similar products, thermoplastic acrylic metal coating resins with a Tg of 90–110°C are ideal.

To meet the high-performance requirements of h.ABS plastic coatings, the glass transition temperature (Tg) of the acrylic resin should first be designed to be as high as possible—typically in the range of 100 to 110°C.

i. The Tg of the thermoplastic acrylic resin modified by PP plastic primer should ideally be between 50 and 65℃.

(2) Calculation of Tg

Among them, Wn represents the mass fraction of the i-th monomer; Tgn represents the glass transition temperature of the homopolymer corresponding to the i-th monomer, with the unit being K.

Note: The unit for the glass transition temperature Tg is ℃, while the unit used when calculating Tg is K.

This formula’s calculated values have certain reference value, with an error margin of ±5℃.

The general selection of monomers falls into three categories: soft monomers, hard monomers, and monomers with intermediate Tg values. The specific proportions depend on experience and continuous experimentation and adjustment.

(3) Copolymerization Reactivity of Monomers

Resins used in coatings are often copolymers, and when selecting monomers, their copolymerization reactivity must be taken into account. Generally, monomers with higher reactivity tend to homopolymerize easily. To ensure smooth copolymerization, the comonomer ratios in the copolymerization mixture should not differ too greatly. For example, styrene is difficult to copolymerize with vinyl acetate, vinyl chloride, or acrylonitrile.

When it is necessary to copolymerize monomers with significantly different reactivities, one monomer can be added in excess, provided that its reactivity ratio is relatively close to those of the other monomers. Styrene and acrylonitrile are difficult to copolymerize; however, the addition of acrylate monomers can improve their copolymerization behavior.

4. Selection of Initiator

The initiators for solvent-based acrylic resins are mainly of two types: peroxide-based and azo-based.

Peroxides are a class of compounds containing the peroxide group (—O—O—). When heated, the —O—O— bond breaks, splitting into two corresponding free radicals and thereby initiating monomer polymerization.

Peroxide initiators are prone to induction decomposition reactions, and their primary free radicals readily abstract hydrogen, chlorine, or other atoms or groups from the macromolecular chains, thereby introducing side chains into the macromolecular chains and broadening the molecular weight distribution.

Azo compounds are molecules containing an azo group—N=N—, which can decompose under the influence of light and heat, releasing nitrogen gas and generating free radicals in the process.

Azo-based initiators generally do not exhibit induction decomposition reactions, and the resulting macromolecules have a relatively narrow molecular weight distribution.

The initiation activities of commonly used peroxide initiators are shown in the table below:

Product Name Decomposition temperature (℃) corresponding to different half-lives
0.1h 1h 10h
Benzoyl peroxide (BPO) 113 91 71
Dilauroyl peroxide 99 79 61
Tert-butyl peroxypentanoate 113 91 72
Tert-pentyl peroxide-2-ethylhexanoate 111 91 73
Tert-butyl peroxypionate 139 119 100
tert-Butyl perbenzoate (TBPB) 142 122 103
Tert-butyl peroxide-3,5,5-trimethylhexanoate 135 114 94
Tert-butyl hydroperoxide (TBHP) 207 185 164
Isopropylbenzene peroxide 195 166 140
Di-tert-butyl peroxide (DTBP) 164 141 121
Dicyclohexyl percarbonate 76 59 44
Diphenyl percarbonate (2-ethylhexyl ester) 80 61 44

There are relatively few varieties of azo initiators; the commonly used ones include azobisisobutyronitrile (AIBN) and azobis(2-methylbutyronitrile) (ABVN).

Product Name Decomposition temperature (℃) corresponding to different half-lives
0.1h 1h 10h
Azobisisobutyronitrile 114 82 64
Azobisisoheptanenitrile 98 75 51

Select an initiator with an appropriate half-life based on the polymerization temperature and the polymerization rate of the monomer. Typically, the half-life of the main initiator at the polymerization temperature should be between 0.5 and 2 hours. Sometimes, a lower-activity initiator can be used in combination; such an initiator usually has a half-life ranging from 2 to 4 hours. Combined initiators are generally employed when the reaction system contains two monomers with significantly different reactivity levels, or in certain special systems with relatively high reaction temperatures—such as automotive touch-up paints.

Method of adding the initiator: In solution polymerization, it is common to mix the initiator with the monomer and add them dropwise. After the monomer addition is complete, after maintaining the temperature for several hours, an additional dropwise addition—either once or several times—is required to completely remove the initiator, thereby maximizing the conversion rate. The amount of initiator used each time should be 10% to 30% of the initial dosage.

5. Selection of Solvents

Common solvents include benzene-based compounds, esters, ketones, and alcohols. Their solubility, arranged from highest to lowest, is as follows: ketones > esters > benzene-based compounds > alcohols.

a. Solvents used in eco-friendly coatings must not contain “three benzenes”—benzene, toluene, and xylene—and typically consist primarily of mixed solvents such as ethyl acetate, butyl acetate (BAC), and propylene glycol methyl ether acetate (PMA).

b. Hydroxyacrylic resins used for amino baking varnishes can be formulated using xylene and butanol as mixed solvents; sometimes, certain butyl cell solvents (BCS, butyl glycol ether, PMA, ethylene glycol ethyl ether acetate—CAC) are also incorporated.

c. In addition to the solvents mentioned above, thermoplastic acrylic resins can also be dissolved using ketone solvents such as acetone, methyl ethyl ketone (MEK), and methyl isobutyl ketone (MIBK).

Generally, mixed solvents with different boiling points are selected based on the reaction temperature.

6. Molecular weight regulator

A molecular-weight regulator can abstract an atom or group from a long-chain radical, causing the long-chain radical to transform into a dead macromolecule while regenerating a free radical that retains initiating and propagating activity. Therefore, a good molecular-weight regulator only reduces the degree of polymerization or molecular weight without affecting the polymerization rate.

Therefore, in order to control the molecular weight, it is necessary to add a molecular-weight regulator. Currently, commonly used regulators are thiol compounds, such as n-dodecyl mercaptan, sec-dodecyl mercaptan, tert-dodecyl mercaptan, and 2-mercaptoethanol (HOCH2CH2SH), among others.

Thiols generally have an unpleasant odor, and their residues can adversely affect sensory evaluation; therefore, their usage must be carefully controlled—typically kept below 1%. Currently, there are also some low-odor transfer agents available, such as the dimer of methylstyrene.

In addition to using molecular-weight regulators to reduce molecular weight, increasing the amount of initiator, raising the reaction temperature, and extending the feed time during the mixing stage—provided that the formulation allows—can all help lower the molecular weight to some extent.

7. Basic Process Flow

Basic equipment requirements:

Polymerization reactors typically use stainless steel or enameled glass reactors equipped with a jacket. Heat exchange is achieved through the jacket, allowing for heating, removal of polymerization heat, or cooling of the reaction mixture. In addition, these reactors are fitted with a stirrer and a reflux condenser, as well as feed ports for monomers and initiators, and inlet and outlet ports for inert gases.

The basic process is as follows:

(1) Mixing of comonomers. The key lies in accurate measurement: whether it’s a major ingredient (such as hard or soft monomers) or a minor ingredient (such as functional monomers, initiators, molecular weight regulators, etc.), it’s best to achieve accuracy within ±0.2%. This ensures precise implementation of the formulation. At the same time, the mixture should be prepared and used immediately.

(2) Add the batch material to the reactor. Add the prescribed amount of (mixed) solvent to the reaction vessel, gradually heat it up to the reflux temperature, and maintain this temperature for about 0.5 hours to remove oxygen.

(3) At the reflux temperature, add the mixed solution of monomer and initiator dropwise according to the process requirements. The addition rate must be uniform; if the system temperature rises too rapidly, reduce the addition rate.

(4) Thermal polymerization. After the monomer has been added dropwise, maintain the reaction at an elevated temperature for a specified period to allow further polymerization of the monomer.

(5) Post-elimination: After the insulation period ends, the initiator can be added in two or more separate batches at intervals to increase the conversion rate.

(6) Re-apply insulation. During the later stages of insulation, you can slightly increase the temperature as needed.

(7) Sampling and analysis. The main indicators measured include appearance, solid content, and viscosity, among others.

(8) Adjust indicators;

(9) Filtration, packaging, quality inspection, and warehousing.

Supplement:

(1) The basic advantages of acrylic coatings include excellent weather resistance, outstanding gloss retention and color fastness, as well as good resistance to water, acids, and alkalis. However, they also have certain drawbacks: low solid content, poor film leveling, susceptibility to brittleness and cracking at low temperatures, tendency to become sticky at high temperatures, poor solvent release, relatively slow drying time, and inadequate resistance to solvents.

(2) Introduce n-butyl methacrylate or isobutyl methacrylate, tert-butyl methacrylate, lauryl methacrylate, stearyl methacrylate, and acrylonitrile to enhance solvent resistance.

(3) Introducing polar monomers such as acrylic acid, methacrylic acid, and hydroxyacrylates can improve the resin's wettability toward pigments and fillers.

(4) Adding an appropriate amount of nitrocellulose or cellulose acetate butyrate can significantly improve the solvent release properties of the coating, its leveling performance, and the orientation of aluminum flakes in metallic effect paints.

(5) The leveling property of the coating film can be improved by reducing the molecular weight of the copolymer.

III. Acrylic Resin Production Technology

Reference: Jiangsu Sanmu Group — Acrylic Resin Production Technology Training

1. Introduction to Acrylic Resin Production

(1) Acrylic resin production process

Acrylic resin production involves multiple stages, including formulation and process design, control of raw materials used in synthesis, equipment and process conditions, measurement and instrumentation, production operations, intermediate control, quality inspection, and packaging.

(2) Introduction to Common Issues in Acrylic Resin Production

Reversible—For example, in production, certain abnormal phenomena may occur, such as excessively high or low solid content or viscosity of acrylic resin, strong odors, or low monomer conversion rates. By taking effective corrective measures, products that initially fail to meet the specified standards can be brought into compliance.

Irreversible—The resin exhibits a darker color, leaning toward yellow or reddish hues. The resin product appears whitish, milky, or cloudy. The resin also shows poor flowability and may contain gel-like substances or gel particles.

2. Control over the raw material stage in acrylic resin production

(1) Types and Requirements of Initiators

BPO (Benzoyl Peroxide)

a. It is best to choose products with a content of 70-75%. BPO with a content exceeding 98% carries an explosion risk when used. Additionally, the BPO content indicated on the formulation must be flexibly adjusted during actual production based on its specified level.

b. If BPO is stored for an excessively long time (e.g., more than 6 months), both the moisture content and active oxygen levels within the product will decrease. Resins produced using such an initiator tend to turn yellow, failing to meet the appearance requirements of being water-white and transparent.

(2) Acrylic monomer

These monomers—such as butyl acrylate BA, styrene ST, and methyl methacrylate MAA—are not suitable for storage at high temperatures. When stored for extended periods at elevated temperatures, the double bonds of these monomers tend to undergo self-polymerization. In mild cases, this results in the formation of fine, tiny particles (giving the liquid a milky appearance), flocculent aggregates; in severe cases, the monomers can gel and solidify completely.

Preliminary Determination and Testing Methods for Monomer Polymer Content:

a. Visually check whether the individual unit appears transparent;

b. Check whether the viscosity of the individual sample is normal and whether any small particles or flocculent substances are present. A more precise method is to use the methanol test.

(3) Introduction to Solvents Used in Acrylic Resins

The solvent has a yellowish color or fails to meet purity standards, such as having an excessively high water content.

After adding all the solvent in the later stage of the reaction, the process typically requires refluxing for 30 minutes. This step is crucial and should not be overlooked—for one thing, it helps remove water; for another, it ensures that the residual monomer/initiator levels in the system are minimized, thus preventing the resin from developing an unpleasant odor.

(4) Introduction to Functional Monomers or Additives

It is essential to strictly control substances such as glycidyl ester of tertiary butyl carbonate (E-10/N-10) and chain regulators (V-276/A-12). Otherwise, these substances could affect the resin’s technical specifications and quality, including its appearance, color, and conversion rate.

(5) Raw Material Control During the Ingredient Mixing Process

a. If, during the feeding process, you notice that some acrylic monomers have a dark color, yellowing, moisture, or foreign substances such as rust, do not proceed with feeding. Otherwise, the resin produced may easily darken or turn yellow, and there could also be milky appearance or gel particles.

b. The reason for emphasizing uniform and moderate-speed addition of the mixed monomers during the reaction is to ensure good heat exchange among the materials.

3. Control of Acrylic Resin Production Equipment and Processes

(1) Reactor Design for Acrylic Resin Production

To ensure sufficient condenser area, in general, a 10 m³ reactor should be equipped with a condenser area greater than 40 m², and a 3 m³ reactor should be equipped with a condenser area greater than 25 m²; otherwise, the condensation effect will be poor.

(2) Producing multiple varieties in a single batch can lead to incomplete cleaning of the pot, which in turn may cause the resin to become cloudy or milky.

When thermoplastic and thermosetting acrylic resins are mixed for production, due to the significant difference in molecular weights and the distinct structures of the resins, their compatibility is poor. Additionally, if the reactor cleaning is incomplete or inadequate—particularly in areas such as pipelines and filters—poor resin miscibility often leads to emulsification and cloudiness in the resin product.

4. During the synthesis of acrylic resin, adjustments and changes in viscosity, solid content, acid value, conversion rate, and other parameters are made.

(1) During central control, if the resin viscosity or conversion rate is found to be unqualified (or too low), the cause should be carefully investigated.

If the materials have not been mixed incorrectly, the initiator should be added as specified, and the reaction should continue under保温 conditions. Samples should be taken again at scheduled intervals for testing. Under normal circumstances, both the solid content and viscosity should increase.

It should be attributed to the ingredients—specifically, too much bottom-layer solvent or insufficient monomer added. The appropriate treatment involves calculating and removing the excess solvent based on the measured viscosity and solid content until the resin meets the specified technical standards. Under these circumstances, the resin can still be salvaged.

(2) During central control, it was found that the resin’s viscosity and solid content were relatively high.

If the equipment checks out fine, there are two possible scenarios: First, the amount of acid may be excessive; this can be confirmed by measuring the acid value of the resin. Otherwise, the issue lies in the formulation process.

Second, if too much of the individual component was added while too little solvent was used, or if the solvent has evaporated, add more solvent.

(3) If the acid value of the resin is found to be too high or too low,

In general, if the amount of acid added is not accurate enough, the acid value can be adjusted by making appropriate changes to the solvent. If there is no room for further adjustment, a new batch can be produced and then the two batches of resin can be mixed together, ensuring that the final product meets the required specifications.

5. Filtration and Packaging Requirements for Acrylic Resins

(1) If impurities, a darker appearance, or water droplets are found after the resin has been placed in the container, the cause must be investigated immediately.

There may be three possible causes for the issue of particles or other impurities:

If the filter bag ruptures during resin filtration or if the filter bag’s mesh size does not meet the required specifications, the resin should be re-filtered. Additionally, the packaging drum is not clean; water has entered the packaging drum; or the original chemicals in the recovery drum have not been thoroughly cleaned out.

(2) Qualified resin must be packaged only after it has cooled down. The bucket lid should not be tightened immediately; otherwise, during transportation while still hot, the large buckets could easily become deformed.

(3) Note: When selecting monomers, you should also pay attention to their toxicity levels.

In general, the toxicity of acrylates is greater than that of their corresponding methyl acrylates—for example, methyl acrylate is more toxic than methyl methacrylate. Moreover, ethyl acrylate also exhibits relatively high toxicity. Among the monomers used in the copolymerization of acrylate monomers, acrylonitrile and acrylamide are highly toxic and require careful protective measures.

Share to:

Related News


Safety and Management of Hazardous Chemicals

Hazardous chemicals refer to substances that are flammable, explosive, toxic, harmful, or radioactive—materials that pose a significant risk of causing personal injury and property damage during transportation, loading and unloading, and storage and custody, thus requiring special protection.


Detailed Explanation of Ceramic Decal Application Technique

In our daily lives, we often see beautifully crafted patterns on ceramic bowls and plates—patterns that are exquisite and incredibly delicate. The floral designs on ceramics are not only heat-resistant but also resistant to chipping and discoloration. But did you know how these intricate floral designs are applied in the first place?


Introduction to UV Absorbers and Their Applications

Ultraviolet absorbers are a class of substances that can prevent the degradation of polymers caused by sunlight or other artificial ultraviolet light; they are a type of light stabilizer. The use of ultraviolet absorbers can effectively protect treated objects from, or at least mitigate, damage to their color. Since different types of polymers are susceptible to degradation at different ultraviolet wavelengths, various ultraviolet absorbers can absorb different wavelengths of ultraviolet light. Therefore, when selecting an ultraviolet absorber, it is essential to take into account the specific type of polymer involved.