Application of UV Resins in Wood and Building Material Coatings
Release time:
2018-04-17 10:37
I. Application Fields
1. Flooring: Solid wood flooring, solid wood composite flooring, bamboo flooring, engineered wood flooring, and PVC resilient flooring;
2. Calcium silicate boards: interior and exterior wall tiles, floor tiles, and skirting boards;
3. Furniture: Solid wood (shaped), wood-veneered MDF, composite board, PVC edge banding, wooden doors (including door frames), aluminum alloy (ceiling).

II. Coating Method
1. Roller coating; 2. Dip coating; 3. Spray coating; 4. Wipe coating; 5. Draw-down coating.

III. Viscosity Reduction Methods
1. Choose a resin with high solids content and low viscosity (narrow range);
2. Select appropriate active monomers (use in large quantities);
3. Select a suitable organic solvent (only for spray application);
4. Paint heating application (continuous circulation).
IV. Drying Method
1. Heating and flow-assisting section: IR at approximately 50℃ with exhaust ventilation;

2. UV Curing: Mercury lamp curing (deep curing in solid-color systems) and LED-UV.

Wood-coating processes generally involve minimal waste of substrate materials; any defective products must be sanded and reworked. Therefore, sandability is a fundamental requirement for coatings. Putty and primer must both be sanded before proceeding to the next coat, while topcoats are applied only to defects that can still be salvaged.
Brittle/hard: Easy to grind; soft/tough: Difficult to grind.
V. UV Coating for Wood Products and Application Map for Boxing Resin (Draft)

6. UV Putty Paint
| Raw materials | Proportion | Process | Note |
| EHKA3777 | 0.3 | Stir well to dissolve the BDK. | 1. The putty is recyclable, and its viscosity can be adjusted according to the roughness of the substrate (1000/3000/5000 cps). For conventional viscosity adjustment, TPGDA is typically used; for rapid viscosity adjustment, HEMA can be selected. 2. The putty should not be reflowed and should have a jelly-like appearance. A small amount of fumed silica can be added to improve thixotropy, making it easier to apply using the upper roller. |
| Tego920 | 0.2 | ||
| 1173 | 2 | ||
| BDK | 1 | ||
| TPGDA | 11.5-20 | ||
| B-522 | 30-40 | High-speed dispersion | |
| B-113 | 10-20 | ||
| Talc powder (1250 mesh) |
20-30 | High-speed dispersion, viscosity measurement, and viscosity adjustment using TPGDA. |
7. UV Roller-Applying Primer
| Raw materials | Proportion | Process | Note |
| EHKA3777 | 0.3 | Dissolve/Disperse Adjust viscosity later by leaving a margin for TPGDA. |
1. Adjust according to the roughness of the substrate (or putty), with viscosities of 2000/3000/5000 cps respectively. 2. Hardened sole: Add B-574C/TMPTA/DPHA as an additional component to improve grindability. 3. Crack-resistant primer: Add B-252/B-302/B-165; 4. Adhesive base: Add B-02/B-535/B-581L/B-506 as an additive. |
| Tego920 | 0.2 | ||
| 1173 | 3 | ||
| B-21 | 3 | ||
| BP | 1 | ||
| HEMA | 4 | ||
| TPGDA | 10-20 | ||
| B-522 | 8-15 | High-speed dispersion | |
| B-113 | 30-40 | ||
| B-165 | 5-8 | ||
| Talc powder | 15-25 | High-speed dispersion, viscosity measurement, and viscosity adjustment using TPGDA. | |
| R972 | 0.2 |
8. UV Roller-Coated Gloss Clear Coat
| Raw materials | Proportion | Process | Note |
| EHKA3777 | 0.2 | Dissolve/Disperse Adjust viscosity later by leaving a margin for TPGDA. |
1. Viscosity: Gravity roller—30–60 seconds (25℃); laser roller—60–90 seconds (25℃); 2. Increase hardness: Replace some of the DPHA with transparent powder; 3. Improve wear resistance: Increase the ratio of B-912/B-601/DPHA; 4. Easy to clean, graffiti-resistant, smoothness improved, and B-868 content increased. |
| Tego920 | 0.2 | ||
| Hand-feel additive | 0.1 | ||
| 1173 | 4 | ||
| B-21 | 2 | ||
| BP | 1 | ||
| HEMA | 5 | ||
| TPGDA | 25-40 | ||
| B-868 | 1-2 | High-speed dispersion | |
| B-302 | 5-10 | ||
| B-912 (or B-601) | 5-8 | ||
| B-113 | 30-40 |
9. UV Spray Gloss Clear Coat
| Raw materials | Proportion | Process | Note |
| EHKA3777 | 0.2 | Dissolve/Disperse | 1. Viscosity at room temperature: 14–20 seconds; 2. Thick coating to prevent cracking: Add more B-302 and reduce B-574C. 3. Anti-sagging for special-shaped parts: Add 5-10% of B-6371-3 or 10% of KN1096F-B. |
| Tego920 | 0.2 | ||
| 1173 | 4.5 | ||
| HEMA | 4 | ||
| TPGDA | 20-30 | ||
| B-113 | 10-15 | High-speed dispersion | |
| B-520 | 25-35 | ||
| B-574C | 10-15 | ||
| B-302 | 6-8 | ||
| B-868 | 2 | ||
| EAC | 10 |
10. UV-coated matte clear topcoat
| Raw materials | Proportion | Process | Note |
| EHKA3777 | 0.3 | Dissolve/Disperse | 1. Excellent transparency, scratch resistance, smoothness, and gloss: 16–18°; adjust the gloss level by blending with B-328M/E-1011. 2. Anti-sagging for irregular-shaped parts: Add 5-10% of B-6371-3/KN1096F-B. |
| Tego920 | 0.2 | ||
| BYK111 | 0.3 | ||
| 1173 | 4.2 | ||
| HEMA | 4 | ||
| TPGDA | 15-25 | ||
| B-328M | 30 | High-speed dispersion | |
| B-912 | 5 | ||
| B-574C | 21 | ||
| B-868 | 2 | ||
| E-1011 | 3 | High-speed dispersion | |
| R972 | 0.2 | ||
| EAC | 10 |
11. UV Roller-Coated Matte Clear Coat
| Raw materials | Proportion | Process | Note |
| EHKA4010 | 0.5 | Dissolve/Disperse | 1. Viscosity: 400-500 cps; 2. Gloss: 28-30° (three-point light). |
| EFKA3777 | 0.2 | ||
| Tego920 | 0.1 | ||
| 1173 | 3 | ||
| B-21 | 2 | ||
| BP | 1 | ||
| HEMA | 3 | ||
| TPGDA | 20 | ||
| B-868 | 2 | High-speed dispersion | |
| B-328M | 25-40 | ||
| B-302 | 5-8 | ||
| B-113 | 15-20 | ||
| BYK991 | 1 | High-speed dispersion | |
| Rad2105 | 3 | ||
| R972 | 0.2 |
12. UV roller-applied white primer
| Raw materials | Proportion | Note |
| EHKA4010 | 0.3 | 1. Viscosity: 1000-2000 cps; 2. Use TPGDA for viscosity adjustment; 3. Typically, apply two to three coats of primer, sanding between each coat. 4. For spray application, dilute HEMA/EAC to a viscosity of 16–20 seconds. |
| Tego920 | 0.1 | |
| 184 | 3 | |
| 819 | 1 | |
| HEMA | 4 | |
| TPGDA | 15 | |
| B-527M | 48.5 | |
| Titanium dioxide | 18 | |
| Talc powder | 10 | |
| R972 | 0.1 |
13. Glossy topcoat with UV laser roller whitening
Pigment paste grinding: L200
| Raw materials | Proportion |
| B-527M | 75 |
| Qin White Powder | 25 |
| EFKA4010 | 1 |
High-gloss white surface:
| Raw materials | Proportion | Process | Note |
| Tego920 | 0.5 | Dissolve | 1. Use 200-mesh filtration; later, use TPGDA to adjust viscosity for 60–90 seconds. 2. Domestic titanium dioxide 2377: L=97; DuPont titanium dioxide 920+: L=98; 3. Glossiness: 92° or higher. |
| 184 | 3 | ||
| 819 | 1.5 | ||
| TPGDA | 15 | ||
| B-375 (B-113) | 12 | High-speed dispersion | |
| L200 | 68 |
14. UV solid wood (wood veneer) hole-filling solvent-free primer for spraying
| Raw materials | Proportion | Note |
| EHKA3777 | 0.5 | 1. Heat and spray within 15–25 seconds; 2. Apply two to three coats according to the thickness of the wood’s vessels, and sand between each coat. |
| Tego920 | 0.3 | |
| BP | 1.2 | |
| B-21 | 2.5 | |
| BDK | 1 | |
| 1173 | 3 | |
| HEMA | 6 | |
| TPGDA | 20 | |
| TMPTA | 10 | |
| B-5225 | 40 | |
| Talc powder (1250 mesh) | 15 | |
| R972 | 0.2 |

Share to:
Related News
A Comprehensive Performance Comparison of Silicone Photocurable Resins
This article presents performance evaluation tests on four silicone UV resins developed by Boxing Company. To help everyone clearly and concisely understand the performance characteristics of these four resins, the tests focus on a parallel comparison of the products’ most fundamental physical properties and performance attributes. We hope these results will be helpful to our customers in selecting the right products and formulating their applications.
Analysis of the PVC Leather UV Roller-Coating Gloss Finish Project
Polyvinyl chloride, abbreviated as PVC in English, is a polymer formed by the free-radical polymerization of vinyl chloride monomer (VCM) under the initiation of initiators such as peroxides and azo compounds, or through the action of light and heat. Homopolymers and copolymers of vinyl chloride are collectively referred to as vinyl chloride resins.
UV LED Technology and Applications
An UV-LED (or UV Light Emitting Diode) is a solid-state semiconductor device that can directly convert electrical energy into ultraviolet light. It is a type of LED with a wavelength range of 10–400 nm, representing monochromatic invisible light typically below 400 nm. The wavelengths commonly used for curing applications are 365 nm and 395 nm. UV adhesives are generally cured using the 365 nm wavelength.